Crack Control of Large Size 4H-SiC Ingot by Nano Laser Cutting –

Crack Control of Large Size 4H-SiC Ingot by Nano Laser Cutting –

PAM-XIAMEN provides services of cutting, grinding, polishing, etc. For SiC wafers, more info please consult: [email protected] 

1. Abstract

Due to the extremely high hardness of SiC, traditional diamond wire saw cutting can easily cause problems such as wide cutting seams, sectional cracks, and surface roughness. Compared with it, laser cutting has become an efficient technology path for processing SiC wafers due to its non-contact and controllable energy characteristics, especially in terms of high material utilization and processing efficiency. Its essence relies on precise induction and orderly connection of cracks. This article focuses on the study of multiple core parameters during nanosecond laser cutting of N-type 4H-SiC, such as laser power, scanning speed, number of repeated scans, and scanning line spacing, and their effects on crack propagation behavior and cutting quality. Based on this, a concise, high-speed, and efficient laser process strategy suitable for large-size SiC ingot slicing was proposed, and the optimal parameter combination for 6-inch, 500μm thick 4H-SiC wafer separation was successfully optimized. The geometric characteristics and residual stress analysis of the polished wafer indicate that the nanosecond laser cutting process did not cause significant abnormalities.

2. Experiment

The experiment selected 6-inch N-type 4 ° skewed 4H-SiC wafer (thickness 350μm) and SiC ingot. The core processing equipment is a nanosecond pulse laser (λ=532 nm, τ=9.7 ns, P=2.9 W, E-max=350 μ J @ 5 kHz, f_rep=1-15 kHz, TEM00, M ²<1.3). Place the SiC sample on an XYZ electric translation stage, achieve laser internal focusing through Z-axis focusing, and scan the XY axis to form a modified layer inside the SiC. Using optical microscopy (OM) and scanning electron microscopy (SEM) to observe the initiation, propagation, and convergence of laser-induced microcracks. The surface morphology of the slice is analyzed by SENSOFAR ® 3D optical profilometer and atomic force microscope (AFM). After chemical mechanical polishing (CMP), the TTV, BOW, and WARP of the wafer were evaluated, and the residual stress of the polished substrate was measured using the photoelastic method.

Fig. 1 (a) 6-inch SiC slice; (b) Optical microscope and AFM images of SiC slice surface

Fig. 1 (a) 6-inch SiC slice; (b) Optical microscope and AFM images of SiC slice surface; (c) Polished SiC wafer; (d, e) Geometric parameter analysis; (f) Stress mapping image obtained by photoelastic method

 3. Conclusion

This article uses nanosecond laser cutting to cut 6-inch N-type 4° off-cut 4H-SiC wafer, focusing on analyzing the effects of laser power, scanning speed, line number, and group spacing on cracks. Optical microscopy (stripe color) and scanning electron microscopy (microcrack width) analysis indicate that the cracks are caused by the volume expansion and thermal stress of the laser modified layer, and the expansion intensifies with increasing power and number of lines.

By optimizing the power and number of lines to control the width of microcracks, and promoting crack interconnection with appropriate spacing between groups, this process significantly reduces the proportion of modified zones, lowers slicing difficulty, reduces debris pollution and material loss, while ensuring production efficiency. Under optimized parameters, a chip with a thickness of approximately 500 μm and a 4° off-cut was successfully cut from a 6-inch N-type SiC ingot. The polished wafer exhibits low TTV, WARP, BOW values, and low stress characteristics. It’s confirmed that nanosecond laser cutting is an effective method for achieving low loss and low-cost manufacturing of large-sized SiC wafer, and is suitable for processing large-sized SiC ingots.

powerwaywafer

Whether you need SiC wafer for research or for industrial applications, please contact us email at [email protected] and [email protected].

 

Reference:

Yu, X., Wu, W., Li, B., Xiu, X., Zheng, Y., & Zhang, R. (2025). Crack control for efficient nanosecond-laser slicing of large-size 4H-SiC crystals. Applied Surface Science, 697, 163014.