Study on the Influencing Factors and Regulation Mechanisms of Mechanical Strength of Float-Zone Silicon Wafers +

Study on the Influencing Factors and Regulation Mechanisms of Mechanical Strength of Float-Zone Silicon Wafers +

With the growing demand for low-power, high-efficiency power semiconductor devices in fields such as new energy vehicles and rail transportation, power devices like insulated gate bipolar transistors (IGBTs) have attracted widespread attention. The formation of oxygen precipitates must be avoided in IGBT manufacturing; therefore, float-zone (FZ) silicon wafers with extremely low oxygen concentrations are commonly used. However, due to the lack of pinning effect of interstitial oxygen atoms on dislocation motion in FZ silicon wafers, once dislocation sources such as scratches are introduced during processing, slip dislocations can easily propagate during heat treatment, leading to issues like wafer warpage, current leakage, and photolithographic misalignment.

Ion implantation, a core doping technique in semiconductor processing, introduces irradiation damage into silicon wafers. The secondary defects formed after annealing of this damage can significantly reduce the mechanical strength of the wafers. For FZ silicon wafers, whether their inherently lower initial strength exacerbates this problem, and how the unique oxygen concentration distribution of FZ wafers affects their slip resistance, are scientific issues that urgently need to be addressed. Starting from the material characteristics of FZ silicon wafers, researchers have conducted in-depth analyses of the influencing factors and mechanisms of mechanical strength of FZ wafers, aiming to provide theoretical guidance for strength regulation of FZ wafers in power device processing.

1. Material Characteristics and Strength Fundamentals of FZ Silicon Wafers

FZ silicon wafers are prepared by the float-zone melting method and have an extremely low oxygen concentration. According to the study by Takata et al., the oxygen concentration in the FZ silicon wafers used in the experiments is no higher than 0.1×10¹⁷cm⁻³, while that in CZ silicon wafers is no higher than 12.8×10¹⁷cm⁻³. Interstitial oxygen atoms can hinder the growth and extension of dislocations in silicon crystals; therefore, the dislocation mobility in FZ silicon wafers is much higher than that in CZ wafers, exhibiting lower mechanical strength. This characteristic makes FZ silicon wafers more prone to slip from defects such as scratches and undergo plastic deformation when subjected to thermal or mechanical stress.

In high-temperature three-point bending tests, researchers apply stress to obtain stress-strain curves, using the upper yield stress as an indicator to evaluate wafer strength. For FZ silicon wafers, the initial upper yield stress is significantly lower than that of CZ wafers, which is directly related to their low oxygen concentration.

2. Effect of Ion Implantation on the Strength of FZ Silicon Wafers

2.1 Formation of Secondary Defects and Strength Degradation Mechanism

Takata et al. systematically investigated the defect evolution and strength changes in silicon wafers after phosphorus ion and (BF₂)⁺ ion implantation. Transmission electron microscope observations show that, regardless of whether the substrate is CZ or FZ, the morphology of secondary defects formed after implantation of the same ions is essentially the same. For phosphorus ion implantation, dislocation loops called “end-of-range” defects are formed after annealing, with a size of about 10nm. For (BF₂)⁺ ion implantation, dislocation loops parallel to the crystal plane and {111} dislocation loops are formed, with defect sizes reaching 20–150nm and a more widely distributed region. The stress-strain curves reveal a key phenomenon: the upper yield stress of unimplanted samples and as-implanted (without annealing) samples is almost identical, while the strength of annealed samples decreases significantly. This indicates that primary damage such as amorphous layers and point defects do not directly cause strength reduction; rather, the secondary defects formed after annealing are the fundamental cause of strength degradation.

Fig. 1 Stress-strain curves obtained from three-point bending tests at 750°C for phosphorus-implanted samples

Fig. 1 Stress-strain curves obtained from three-point bending tests at 750°C for phosphorus-implanted samples

2.2 Comparison of Strength Degradation Behavior between FZ and CZ Silicon Wafers

Takata et al. compared the changes in upper yield stress as a function of dose for CZ and FZ wafers after phosphorus ion and (BF₂)⁺ implantation. They found that the absolute strength of FZ wafers is approximately 10–15MPa lower than that of CZ wafers, which is attributed to the lack of interstitial oxygen pinning. However, the rate of strength decrease with dose is exactly the same for both: linear decrease under phosphorus implantation, and a sharp decrease in the low-dose region (0 to 1×10¹⁴cm⁻²) followed by a linear attenuation stage under (BF₂)⁺ implantation.

Fig. 2 Relationship between ion dose and upper yield stress: (a) phosphorus ion implantation; (b) (BF₂)⁺ ion implantation

Fig. 2 Relationship between ion dose and upper yield stress: (a) phosphorus ion implantation; (b) (BF₂)⁺ ion implantation

Although the oxygen concentration of the substrate determines the absolute strength level of the wafer, the weakening effect of secondary defects on strength is independent of oxygen concentration and depends only on the type and dose of implanted ions. Further studies show that as the (BF₂)⁺ dose increases, the number of secondary defects increases while their size changes little, explaining the stage of linear strength decrease with dose.

Fig. 3 Cross-sectional transmission electron microscope images of CZ silicon wafers implanted with different doses of (BF₂)⁺ ions and heat-treated

Fig. 3 Cross-sectional transmission electron microscope images of CZ silicon wafers implanted with different doses of (BF₂)⁺ ions and heat-treated: (a) 1×10¹⁴cm⁻²; (b) 5×10¹⁴cm⁻²; (c) 1×10¹⁵cm⁻²

3. Regulation of Critical Shear Stress by Surface Oxygen Concentration in FZ Silicon Wafers

3.1 Scratch-Induced Slip Behavior and Temperature-Independent Critical Stress

During IGBT manufacturing, scratches inevitably occur on the backside of silicon wafers, acting as dislocation sources. Fujise et al. introduced indentations (load 0.98N) on the surface of FZ silicon wafers using a Vickers hardness tester to simulate scratches, and studied the critical conditions for slip generation by high-temperature three-point bending tests. The study found that the critical shear stress is independent of the stress holding time—once the applied stress exceeds the critical value, slip begins to propagate and does not stop automatically.

Fig. 4 X-ray topography images after three-point bending tests at 1023K with different stress holding times: (a) 3h; (b) 5h; (c) 7h

Fig. 4 X-ray topography images after three-point bending tests at 1023K with different stress holding times: (a) 3h; (b) 5h; (c) 7h

In the temperature range of 973–1123K, the critical shear stress of FZ silicon wafers is approximately 1.3MPa, showing a clear temperature independence, indicating the presence of non-thermally activated long-range obstacles. This phenomenon cannot be explained by the classical oxygen pinning theory—when the oxygen concentration is no higher than 1×10¹⁷cm⁻³ and the temperature is no lower than 1123K, the oxygen pinning stress should not exceed 0.5MPa. Therefore, the experimentally observed critical stress of 1.3MPa suggests that other long-range obstacles (such as intrinsic point defect clusters or residual stress fields) exist in FZ silicon wafers, providing non-thermally activated hindrance to dislocation motion.

Fig. 5 Variation of critical shear stress with test temperature

Fig. 5 Variation of critical shear stress with test temperature

3.2 Strengthening Effect of Inward Diffusion of Surface Oxygen

Although the overall oxygen concentration of FZ silicon wafers is extremely low, high-temperature pre-annealing can cause oxygen atoms to diffuse inward from the surface, forming an oxygen concentration gradient in the near-surface region. Fujise et al. pre-annealed FZ silicon wafers at 1373K and 1423K for durations ranging from 30 minutes to 5 hours, and then performed three-point bending tests. The results showed that high-temperature, long-duration pre-annealing significantly improved the slip resistance of FZ silicon wafers.

Fig. 6 Changes in critical shear stress under different pre-annealing conditions

Fig. 6 Changes in critical shear stress under different pre-annealing conditions

By measuring the depth distribution of oxygen concentration below the surface using secondary ion mass spectrometry, and combining it with the empirical relationship between pinning stress and oxygen concentration, the depth range for slip generation was deduced to be 3.3–7.3μm. Dark-field transmission electron microscope images show that in the near-surface region within 3.3μm, dislocation density is high and dislocations are entangled with each other; while in the range of 3.3–7.3μm, dislocation density decreases with increasing depth, and slip is more likely to occur in this region. Furthermore, the study confirmed that at the same depth (5.6μm), the critical shear stress is proportional to the oxygen concentration.

Fig. 7 Depth distribution of oxygen concentration in the surface area of Si wafer after pre annealing conditions

Fig. 7 Depth distribution of oxygen concentration in the surface area of Si wafer after pre annealing conditions

Fig. 8 Transmission electron microscopy dark field image

Fig. 8 Transmission electron microscopy dark field image

Therefore, for low-oxygen-concentration FZ silicon wafers used in IGBT manufacturing, appropriate high-temperature pre-annealing to diffuse oxygen inward can significantly increase the pinning stress in the near-surface region, thereby effectively suppressing slip generated from backside scratches during subsequent heat treatment, and reducing the risks of wafer warpage and current leakage.

The absolute strength of FZ silicon wafers is lower than that of CZ wafers, but the rate of strength decrease with ion implantation dose depends only on the type of implanted ions and is independent of oxygen concentration. By diffusing surface oxygen inward through high-temperature pre-annealing, the critical shear stress can be increased from 2.5MPa to 5.9MPa, which is an effective approach to suppress scratch-induced slip and improve the mechanical reliability of FZ silicon wafers.

Whether you need Silicon wafers for research or for industrial applications, please contact us email at [email protected] and [email protected].

 

References:

  1. Takata, K., Fujise, J., Ko, B., Ono, T., & Tanaka, M. (2022). Effect of ion implantation on mechanical strength of silicon wafers. Japanese journal of applied physics, 61(4), 045503.
  2. Fujise, J., Ko, B., Ono, T., & Tanaka, M. (2020). Effect of Surface Oxygen Concentration on Wafer Strength in Floating Zone Si Wafers. ECS Journal of Solid State Science and Technology, 9(10), 104002.

has been added to your cart.